Welding Glossary
1. Occupational safety.
a. Hazards.
As a general rule, welding almost always involves strong currents or explosive gases, toxic exhaust fumes, dangerous light and heat generation, and splashes of liquid metal. The risks depend on which welding process is used. Welding fumes often contain carcinogenic substances. This is always the case, especially when welding high-alloy materials. The use of welding filler materials containing chromium and/or nickel in the form of chromates and/or nickel compounds also produces carcinogenic fumes. Acute poisoning caused by inhalation of dusts with a very high manganese content can lead to inflammatory reactions in the lungs. This toxicity manifests as bronchitis and may progress to fibrous lung disease. If the extraction system is used correctly, the limit value for manganese and its compounds will not be exceeded. Nevertheless, a special health examination of the lungs is required for welding personnel on a regular basis in accordance with (G39).
In Germany, the TRK limit values for heavy metals must be observed. Many other components are also harmful and must be assessed accordingly (TRGS403, MAK values). TRGS 528, which replaced BGR 220 (welding fumes), regulates, among other things, the requirements for the welding workplace.
b. Measures.
A risk assessment must be prepared for welding workplaces. All components of the welding fume must be taken into account here, including titanium dioxide, fluorides, magnesium oxide, calcium oxide, iron oxides and their alloy components such as nickel, cobalt, chromium and manganese. With high-alloy steels, electrode welding should, if possible, be avoided in favour of gas-shielded welding or automated processes, as fewer chromates are released due to the lack of a coating on the electrode. According to the Occupational Safety and Health Act (ArbSchG), appropriate expert instruction is mandatory for all employees; furthermore, proof of training (skilled worker certificate or course examination from a chamber of crafts) is common. In many industrial sectors and in railway applications, welding supervision is required.
In oxyfuel welding, protective glasses are needed so that no glowing parts or sparks get into the eyes. The lenses are tinted so that the welding area can be observed without glare.
Arc welding produces ultraviolet radiation that damages the skin, and especially the eyes.
Furthermore, infrared radiation (heat radiation) is produced, which not only causes burns on unprotected parts of the body, but can also damage the retina.
Therefore, protective glasses must be used that shield both types of radiation. The protection classes for such glasses are specified in the European standard EN 169. Protection classes 2 to 8 are specified for oxyfuel welding, while classes 9 to 16 are intended for open arc welding. The protective glasses carry a label that characterizes the properties of the glass. The information is as follows: protection class, manufacturer's code, optical class 98, DIN standard. The modern replacement for protective glasses is the automatic welding protection filter.
Since UV radiation also damages the skin, a shield is used that covers the entire face. In front of the actual, almost black glass, there is usually a normal glass, which keeps out sparks and is cheaper to replace. In order to have both hands free, the shield can be attached in a folding manner to a protective helmet or a device worn on the head. In addition, special flame-retardant welding clothing must be worn that safely covers all areas of the skin. Many welding processes are very loud, so appropriate hearing protection is necessary.
Welding also creates the finest dust particles that have to be extracted so that they do not get into the welder's lungs and from there diffuse into the bloodstream. For this purpose, mobile or stationary welding fume filters are used to extract and filter this fine dust. The state of the art today is so-called ePTFE filters (surface filtration). If effective extraction of welding fumes cannot be ensured, the welder must be protected by personal protective equipment in the form of a powered air-purifying respirator (PAPR). These devices do not protect against a lack of oxygen or harmful gases in shafts and containers. If adequate ventilation is not possible, self-contained breathing apparatus must be worn. Particular caution is required when flame straightening and preheating with gas burners in inadequately ventilated, confined spaces, as the flame consumes some of the oxygen needed for breathing.
When welding, people in the surrounding area must also be protected from radiation and noise. For this there are welding curtains and strip curtains as well as soundproof partition systems. When carrying out manual arc welding, particular attention must be paid to the electrical hazard to the welder. Although the arc voltage is below the generally dangerous range, a number of precautionary measures must be observed, especially when working under particular electrical hazard, for example in narrow electrically conductive spaces (boilers, pipes, etc.); these are suggested, among other places, in the information sheet BGI 553 of the metal trades employers' liability insurance association.
In laser welding, the laser beam itself is an additional source of danger. It is usually invisible. While near-infrared radiation (solid-state laser, fiber laser, diode laser) penetrates the skin and the eye and causes retinal damage even at low intensities (scattered radiation), the radiation from the CO2 laser (mid-infrared) is absorbed on the surface (skin and cornea of the eye) and causes superficial burns. Skin burns caused by near-infrared lasers are also dangerous, among other reasons because the radiation is absorbed in deep areas under the skin where there are no temperature-sensitive nerves. Laser welding machines are usually safely enclosed (interlocked protective doors, laser protective windows); they then fall under laser class I and can be operated safely without laser safety glasses.
2. Electrode welding and arc welding.
Manual metal arc welding (MMA welding, EN ISO 4063: Process 111) is one of the oldest electrical welding processes for metallic materials that is still used today. In 1891, Nikolai Gavrilovich Slavyanov replaced the carbon electrodes that had previously been used for arc welding with a metal rod that was both arc carrier and filler. Since the first stick electrodes were not coated, the weld was not protected from oxidation. Therefore, these electrodes were difficult to weld with.
An electric arc between an electrode that melts as filler material and the workpiece is used as a heat source for welding. The high temperature of the arc melts the material at the weld. Welding transformers (stray field transformers) with or without welding rectifiers, welding converters or welding inverters serve as welding power sources. Depending on the application and electrode type, welding can be carried out with direct current or alternating current.
Coated stick electrodes, for example for unalloyed steels according to ISO 2560-A, develop gases and welding slag when melted. The gases from the coating stabilize the arc and shield the weld pool from oxidation by atmospheric oxygen. The welding slag has a lower density than the melt, floats onto the weld seam and provides additional protection of the seam against oxidation. Another desired effect of the welding slag is the reduction of welding shrinkage stresses due to the slower cooling, as the component has more time to reverse the plastic deformation.
The electron bombardment causes the anode (positive pole) to heat up more. In most welding processes, consumable electrodes are operated as anodes, i.e. the workpiece is the cathode (negative pole). For coated stick electrodes, the polarity depends on the electrode coating. If the coating consists of components that are difficult to ionize, as is the case with basic electrodes, the electrode is welded on the hotter positive pole; otherwise, because of the lower current load, on the negative pole.
The main area of application for manual arc welding is steel and pipeline construction. Electrode welding is preferred in the assembly sector due to the significantly lower welding speeds, as the equipment effort is relatively low compared to other processes. Electrode welding can still be carried out without defects even under unfavorable weather conditions, such as wind and rain, which is particularly important for outdoor work. Another advantage is that, in contrast to other processes, the welding can often still be carried out without defects even if the weld joint is not completely bare metal.
3. MIG - MAG welding (gas metal arc welding).
Semi-mechanical gas metal arc welding (GMAW), either as MIG (metal inert gas welding, EN ISO 4063: Process 131) or MAG welding (metal active gas welding, EN ISO 4063: Process 135), is an arc welding process in which the consumable welding wire is continuously fed by a motor at variable speed. The common welding wire diameters are between 0.8 and 1.2 mm (less commonly 1.6 mm). Simultaneously with the wire feed, the shielding or mixed gas is supplied to the weld via a nozzle at approx. 10 l/min (rule of thumb: shielding gas flow 10 l/min per mm of welding wire diameter). This gas protects the liquid metal under the arc from oxidation, which would weaken the weld. Metal active gas welding (MAG) works with either pure CO2 or a mixed gas of argon and small amounts of CO2 and O2 (e.g. "Corgon"). Depending on its composition, the welding process (penetration, droplet size, spatter losses) can be actively influenced; in metal inert gas welding (MIG), the noble gas used is argon, more rarely the expensive noble gas helium. The MAG process is primarily used for steels, the MIG process is preferred for non-ferrous metals.
Alternatively, cored wires, also known as tubular wires, can be used for gas metal arc welding (with active gas EN ISO 4063: Process 136, with inert gas EN ISO 4063: Process 137). These can contain a slag former and, if necessary, alloy additives on the inside. They serve the same purpose as the coating of the stick electrode. On the one hand, the ingredients contribute to the weld volume, on the other hand, they form a slag on the weld bead and protect the seam from oxidation. The latter is particularly important when welding stainless steels, as oxidation, the "tarnishing" of the seam, must be prevented even after the torch has moved on and the shielding gas cover has moved on with it.
History of MIG-MAG processes
GMAW welding was first used in the USA in 1948 in the inert gas or noble gas variant; at that time it was also known as SIGMA welding (shielded inert gas metal arc).
In the Soviet Union, from 1953 onwards, an active gas, namely carbon dioxide (CO2), was used for welding instead of expensive noble gases such as argon or helium. This was only possible because wire electrodes had meanwhile been developed that compensate for the higher burn-off of alloying elements during active gas welding.
In Austria, CMT (Cold Metal Transfer) welding was developed to series-production readiness by 2005, in which the welding current is pulsed and the filler wire is moved back and forth at high frequency in order to achieve targeted droplet detachment with low heat input.
4. Plasma cutter.
The plasma cutter consists of a power source, handpiece, ground cable, power supply line and compressed air supply line. A plasma is an electrically conductive gas with a temperature of around 30,000 °C. The arc is usually ignited with a high-frequency ignition and is constricted at the exit by an insulated, usually water-cooled, copper nozzle. Some systems also use lift-arc ignition, which is also used in TIG welders. With these devices, the torch is placed on the workpiece at the cutting point and a small current flows that is not enough to damage the torch. The gas stream pushes the torch away from the workpiece surface, the arc ignites, and the electronics of the welding power source increase the current to the level required for the cut. Due to the high energy density of the arc, the metal melts and is blown away by a gas jet, creating the kerf. Compressed air is often used as the gas for blowing out. To achieve a better kerf, shielding gas mixtures are also used, which prevent or reduce oxidation. Characteristic of plasma cut kerfs is a rounding of the edge at the entry point.
The process has a number of advantages over other fusion welding processes. In conjunction with TIG pulse welding and TIG AC welding, any material suitable for fusion welding can be joined. TIG welding produces virtually no weld spatter; the health impact of welding fumes is relatively low. A particular advantage of TIG welding is that it does not work with a consumable electrode. The addition of filler metal and the current are therefore decoupled. The welder can optimally adjust the welding current to the welding task and only has to add as much filler as is currently required. This makes the process particularly suitable for welding root passes and for welding in forced positions. Due to the relatively low and localized heat input, the welding distortion of the workpieces is less than with other processes. Because of the high quality of the weld seams, the TIG process is preferred where welding speed is secondary to quality requirements. These are, for example, applications in pipeline and apparatus construction, in power plant construction or in the chemical industry.
The TIG welding system consists of a power source, which in most cases can be switched to direct or alternating current welding, and a welding torch that is connected to the power source via a hose package. The hose package contains the welding current line, the shielding gas supply, the control line and, for larger torches, the supply and return of the cooling water.
5. Plasma welding.
In plasma welding (plasma metal inert gas welding, EN ISO 4063: Process 151), a plasma jet serves as the heat source. Plasma is an electrically conductive gas that is highly heated by an electric arc. In the plasma torch, the plasma gas (argon) flowing through is ionized by high-frequency pulses and an auxiliary arc (pilot arc) is ignited. This burns between the negatively polarized tungsten electrode and the anode designed as a nozzle and ionizes the gas column between the nozzle and the positively polarized workpiece. This makes it possible to ignite the arc without contact. Gas mixtures of argon and hydrogen or argon and helium are commonly used as plasma gas; they protect the melt from oxidation and stabilize the arc. The small additions of helium or hydrogen increase the penetration and thereby the welding speed. The constriction of the plasma by the water-cooled copper nozzle into an almost cylindrical gas column results in a higher energy concentration than with TIG welding, allowing higher welding speeds. The distortion and stresses are therefore lower than with TIG welding. Because the plasma arc burns stably even at the lowest currents (less than 1 A) and is insensitive to changes in the distance between nozzle and workpiece, the process is also used in micro-welding. With the micro plasma welding process (welding current range 0.5-15 A), sheets as thin as 0.1 mm can still be welded. Plasma keyhole welding is used from a sheet thickness of 3 mm and, depending on the material to be welded, can be used for single-pass welding without seam preparation up to a thickness of 10 mm. The main areas of application are container and apparatus construction, pipeline construction and aerospace.
6. Tungsten Inert Gas Welding (TIG).
Tungsten inert gas welding (TIG welding process, EN ISO 4063: Process 141) comes from the USA and became known there in 1936 under the name Argonarc welding. It was only at the beginning of the 1950s that it began to become established in Europe. In English-speaking countries the process is called TIG or GTAW. TIG stands for Tungsten Inert Gas welding and GTAW stands for Gas Tungsten Arc Welding. The word "tungsten" appears in both abbreviations; in German it is called "Wolfram".
There are two ways to ignite the arc: contact ignition and high-frequency ignition.
In the historical contact ignition (scratch ignition), similar to electrode welding, the tungsten electrode is briefly scratched on the workpiece, like a match, thus creating a short circuit. After the electrode is lifted from the workpiece, the arc burns between the tungsten electrode and the workpiece. A major disadvantage of this process is that each time it is ignited, some material from the tungsten electrode sticks and, due to the higher melting temperature of tungsten, remains as a foreign body in the weld pool. Therefore, a separate copper plate lying on the workpiece was often used for ignition.
High-frequency ignition has practically completely replaced scratch ignition. With high-frequency ignition, the gas between the electrode and the workpiece is ionized using a high-voltage pulse generator that applies a high voltage to the tungsten electrode, thereby igniting the arc. The high-voltage pulse generator has a harmless current level.
A variant of contact ignition is lift-arc ignition. The electrode is placed directly on the workpiece at the weld. A small current flows, which is not enough to damage the electrode. When the torch is lifted, the arc ignites and the electronics of the welding machine increase the current to welding amperage. The advantage of this method is that it avoids electromagnetic interference that can occur with high-frequency ignition.
The noble gas argon is usually used for welding, more rarely helium or a mixture of both gases. The relatively expensive helium is used to increase the heat input due to its better thermal conductivity. For austenitic stainless steels, small amounts of hydrogen in the shielding gas can reduce the viscosity of the melt and increase the welding speed (this is then no longer an inert gas, but a reducing gas; see planned change to EN ISO 4063).
The shielding gas is directed through the gas nozzle to the weld. The rule of thumb is: gas nozzle inner diameter = 1.5 × weld pool width. The amount of shielding gas depends, among other things, on the seam shape, material, welding position, shielding gas and nozzle diameter; information on this can be found in the manufacturers' data sheets.
When TIG welding, you can work with or without filler metal. For manual welding, rod-shaped fillers are usually used, as in gas fusion welding. However, confusion with gas welding rods must be avoided at all costs, as their chemical compositions differ.
In TIG welding, a distinction is made between direct current and alternating current welding. Direct current welding with a negatively polarized electrode is used for welding all types of steel, non-ferrous metals and their alloys. In contrast, alternating current welding is primarily used to weld the light metals aluminum and magnesium. In special cases, light metals are also welded with direct current and a positive electrode. Special welding torches with a very thick tungsten electrode and helium as shielding gas are used. The positive polarity of the tungsten electrode is necessary for light metals, as these usually form a hard oxide layer with a very high melting point (as with aluminum oxide, magnesium oxide) on their surface. This oxide layer is broken up when the workpiece is negatively polarized, as the workpiece then acts as an electron-emitting pole and negative oxygen ions are removed.
BGI 746 (Handling tungsten electrodes containing thorium oxide in tungsten inert gas welding (TIG)) contains information on the safe handling of tungsten electrodes containing thorium oxide for tungsten inert gas welding and describes the necessary protective measures to exclude possible hazards from handling these electrodes or to minimize them to an acceptable level. This is necessary because of the low radioactivity of thorium and the harmful dust of the heavy metal. Due to the availability of tungsten electrodes alloyed with lanthanum or rare earths, the use of thorium-alloyed tungsten electrodes can now be dispensed with.
TIG pulse welding
A further development of TIG welding is welding with pulsating current. In TIG pulse welding, the welding current pulsates between a base and a pulse current with variable frequencies, base and pulse current levels and widths. The pulse frequency, pulse width and pulse height can be adjusted separately. TIG pulsing with a variable current curve can only be carried out with a special welding system (welding inverter). The finely adjustable heat input in TIG pulse welding enables good gap bridging, good root welding and good welding in forced positions. Weld seam defects at the start and end of the seam, as in pipe welding, are avoided.
All descriptions refer to manual or partially mechanized TIG welding with filler metal, predominantly ø 1.6 mm. When pulse welding light metals (namely AA6061), melting can be limited to the surface, thus preventing burn-through on thin sheets < 1.0 mm. Especially with fillet welds, the corner is caught more reliably than with standard constant-current welding. Sheets with a thickness of 0.6 mm have also been butt-welded perfectly, as the stability of the arc and the concentrated heat input allow a small, defined weld pool. Tack welding is the main problem when there is a gap and oxygen therefore has access to the root side. The influence of the tungsten electrode alloy and the composition of the shielding gas is important; these parameters significantly influence the process.
7. Purpose of welding.
When defining the term, a distinction is made between joint welding and surfacing (build-up) welding depending on the purpose of welding. Joint welding is the joining (DIN 8580) of workpieces, for example with a longitudinal pipe seam. Surfacing is the coating (DIN 8580) of a workpiece by welding. If the base material and the applied material are different, a distinction is made between surfacing of armor, cladding and buffer layers.
Fusion welding is welding with a localized melt flow, without the application of force, with or without a similar filler (ISO 857-1). In contrast to soldering, the liquidus temperature of the base materials is exceeded. In principle, all materials that can be converted into the molten phase can be joined by welding. Welding is most often used for the material-bonded joining of metals, thermoplastics or glass, both in consumer products and for connecting glass fibers in communications technology. Depending on the welding process, the joint is made with a weld seam or a weld spot, or with friction welding also over an area. The energy required for welding is supplied from outside. The term path welding is used when robots are used for automated welding.
a. Influence of the weld on the base material.
The base material can develop disadvantageous properties due to the welding heat and the subsequent relatively rapid cooling. Depending on the material and the cooling process, hardening or embrittlement can be caused, for example. In addition, high residual stresses can arise in the transition between the weld seam and the base material. This can be countered by a variety of measures in production. These include welding measures, such as the selection of suitable welding processes, filler materials and weld post-treatment processes, preheating of the workpiece, as well as design and manufacturing measures, such as the correct welding and thus assembly sequence, selection of suitable seam shapes and, if there is an option, selection of the right base material.
b. Life extension through post-treatment methods.
The fatigue strength and service life of dynamically loaded, welded steel structures is in many cases determined by the weld seams, especially the weld transitions. Through targeted post-treatment of the transitions by grinding, blasting, shot peening, high-frequency hammering, etc., the service life of many constructions can be significantly increased using simple means.
c. Weldability of steel.
Steels with a carbon content of more than 0.22% are only considered weldable to a limited extent; additional measures such as preheating are required. However, the carbon content of the steel alone does not determine weldability, as this is also influenced by many other alloying elements. The carbon equivalent (CEV) is therefore taken into account for the assessment. For many components, depending on the design and material, additional measures such as preheating or slow cooling, stress-relief annealing or buffer welds are required to avoid cracking and fractures (lamellar tearing). In general, high-alloy or higher-alloy steels are more difficult to weld and require special knowledge and controls from the fabricator. This is one of the reasons why, in addition to the mandatory certified welders, a responsible welding supervisor is appointed in all companies. Without an appointment, the company owner is automatically the liable welding supervisor. From class B onwards, specially trained welding specialists, such as welding engineers/technicians, must be employed to ensure the necessary technical support for the welding work.